Fiber carbon na motatsarin samar da kayan daki na ciki da waje
Yankan:Cire kayan aikin da aka yi da carbon fiber prepreg daga injin daskarewa, yi amfani da kayan aikin don yanke carbon fiber prepreg da fiber kamar yadda ake buƙata.
Layukan:A shafa sinadarin sakin fuska a kan mold ɗin don hana blank ɗin mannewa a kan mold ɗin, sannan a shafa manne da zare na carbon da aka yanke a cikin mold ɗin, sannan a shafa a cikin injin tsabtace iska sannan a aika shi zuwa tankin mai zafi.
Ƙirƙira:Fara tankin matsi mai zafi, dumama wutar lantarki zuwa 150°C, warkarwa na tsawon awanni 3, cire mold ɗin, sanyaya ta halitta na minti 10 zuwa zafin ɗaki, cire mold ɗin don samun gurɓatattun abubuwa.
Gyaran:Karɓi guraben gyare-gyare, yi amfani da almakashi, wuka da sauran kayan aiki don cire gefuna da ba a saka ba na gyare-gyare da hannu, kuma wasu daga cikin samfuran suna buƙatar a tsaftace su akan injin CNC.
Sanding:Sandblasting sanding don inganta ingancin feshi, yana buƙatar yin tauri a saman abin da aka ƙerakayan fiber na carbonamfani da injin rufewa mai amfani da yashi mai ƙarfi a samanzare na carbon, don ƙara kauri, domin biyan buƙatun mataki na gaba na fesawa.
Cikowa:Kayayyakin da aka gama da su waɗanda suka dace da saman da aka yi amfani da shi bayan an yi amfani da yashi, ana kai su kai tsaye zuwa tsarin samarwa na gaba; samfuran da aka gama da su waɗanda suka manyan ramukan yashi a saman suna buƙatar a cika su da resin da hannu (wanda galibi ya ƙunshi resin epoxy da dicyandiamide) don su yi laushi, sannan a kai su tsarin samarwa na gaba bayan an gama resin gaba ɗaya a zafin ɗaki (yana ɗaukar awanni 4-5).
Haɗa fenti, fesawa, busarwa, da busarwa:Kafin fesawa, ana buƙatar a haɗa fenti, rabon haɗuwa shine varnish: taurare = 2:1 (rabo mai nauyi), fenti mai tushen ruwa: ruwa = 1:1 (rabo mai girma). A cikin rumfar fenti bisa ga daidaitaccen fenti mai fesawa (kauri mai ruwa na fesawa na 75μm, yana taka rawa wajen ƙara haske da bayyananniya na samfurin); bayan kammala aikin fesa fenti, za a aika keken zuwa ɗakin busarwa don a sanyaya shi a busar da shi zuwa busarwa ta saman (aƙalla mintuna 30); busarwa ta saman bayan an cire na'urar ratayewa, za a aika samfurin zuwa ɗakin busarwa, a yi amfani da busarwa ta lantarki, a busar da shi a zafin digiri 80 Celsius na tsawon awanni 2.
Kyawun samfurin:Kyawun samfura shine duba ingancin fesawa, galibi ta amfani da lura da ido tsirara, an gano cewa saman fesawa samfurin yana da tabo na ƙura da sauran lahani, buƙatar yashi da goge samansa, yashi don busasshen yashi da kuma yashi mai laushi.
Busasshen yashi:amfani da injin gogewa da gogewa a kan ramin samfurin, yin yashi mai kyau har zuwa saman santsi.
Yashi mai laushi:A cikin teburin yashi, ta gefen fesa ruwa da niƙa, saman samfurin zai kasance ƙuraje masu kyau don niƙa.